Sheet Metal Forming and Stamping
What You'll Learn
- 1Compute blanking force from shear perimeter and stock shear strength
- 2Develop a flat blank using bend allowance and the K-factor
- 3Predict springback angle from yield strength and bend geometry
- 4Set punch clearance and blank holder force for a drawing operation
A flat pattern that folds perfectly in software often springs open several degrees on the press brake, and a deep-drawn cup that looked fine in CAD tears at the punch nose on the first hit. Sheet forming is governed by elastic recovery, the location of the neutral axis, and the ratio of blank size to punch diameter, none of which appear in a solid model. This lesson gives the arithmetic for punch force, blank development, and springback, then shows how clearance and blank holder force decide whether a draw wrinkles or tears.
Theory and Foundations
Sheet operations fall into three families: cutting, where the sheet is sheared through its thickness; bending, where the sheet is rotated about an axis without changing its thickness appreciably; and drawing, where an annular flange is pulled into compression and converted into a wall. The assumptions used below are plane stress through the thickness, constant sheet thickness except where noted, and a rigid-perfectly-plastic material for force estimates, with elasticity retained only for springback.
Cutting force scales with the sheared edge, not with part area. For a hole of diameter punched through thickness with shear strength ,
where is the perimeter of the cut. Clearance is applied per side as a fraction of thickness,
with near 0.06 for aluminum, 0.08 to 0.10 for soft steel, and 0.10 to 0.12 for stainless. Too little clearance work-hardens the edge and doubles punch wear; too much rolls a heavy burr and pulls a secondary slug.
Bending is a neutral-axis problem. During bending the outer fibers extend and the inner fibers compress, and somewhere between them lies a fiber of unchanged length called the neutral fiber. The K-factor locates it:
The arc length of the neutral fiber is the bend allowance:
with the inside bend radius. Blank development then uses the outside dimensions of the part. The outside setback and bend deduction are
so that the flat blank length equals the sum of the outside leg lengths minus the bend deduction.
Springback is the elastic energy stored in the bent region that is released when the punch lifts. For an elastic-perfectly-plastic sheet the plastic moment per unit width is and the elastic section modulus is , so the curvature released on unloading is
and the angle recovered is that curvature change times the length of the bent arc,
with the neutral radius. The relation is linear in yield strength and inversely proportional to thickness, which is exactly why high-strength steel and thin gauge spring back so much more than mild steel.
Drawing converts an annular flange into a cup wall, and the governing ratio is the draw ratio:
where the limit draw ratio is about 2.0 to 2.1 for deep drawing steel, 1.8 for aluminum, and 1.7 for stainless. Past the limit the cup thins and tears at the punch nose. Blank holder force sits in a narrow window: high enough to stop the flange wrinkling, low enough to let the metal flow,
which is why the holder is usually regulated by gas springs rather than by press tonnage.
Key Formulas
Minimum bend radius also follows the same geometry, since the outer fiber strain in a bend is
so cracking is avoided by keeping below the elongation of the sheet in the transverse direction, which is why a bend run across the rolling direction survives a radius that would split a bend run parallel to it.
Worked Examples
| Operation | Key parameter | Typical value | Common defect |
|---|---|---|---|
| Blanking | Clearance per side | 6 to 12 percent of t | Burr, secondary slug |
| Bending | Inside radius | 1 to 2 times t | Springback, cracking |
| Drawing | Limit draw ratio | 1.7 to 2.1 | Tearing, wrinkling |
| Flanging | Hole expansion | 25 to 40 percent | Edge splitting |
| Coining | Unit pressure | 2 to 4 times yield | Incomplete detail |
Real-World Examples
- Server chassis - A CR4 panel is blanked and bent on a 12 station progression die at 60 strokes per minute, with 8 percent clearance per side on 1.5 mm stock.
- Door inner - A 0.7 mm aluminum shell is drawn with blank holder force held at 2 percent of cutting force to avoid flange wrinkles without starving the punch nose.
- Can body - A 0.28 mm tinplate shell is drawn in three stages at a draw ratio of 1.8 per stage, each stage below the LDR of 2.0.
- Stainless bracket - A 304 bracket with 2 mm wall is overbent about 5.6 degrees on a 20 mm radius to land at 90 degrees after springback.
đĄMind the Grain Direction
Common Mistakes
Using a K-factor of 0.50 by default
Fix: Start at 0.33 for tight radii and verify the flat on one physical sample before releasing the die.
Setting blank holder force from press size
Fix: Start near 2 percent of cutting force and adjust until wrinkles and tears both stop.
Ignoring springback on high-strength steel
Fix: Overbend by the computed angle and re-measure, since springback scales with yield strength.
Key Takeaways
- Blanking force scales with shear perimeter times thickness times shear strength
- Bend allowance uses the neutral axis, where K rises from about 0.33 toward 0.50
- Springback curvature is three times yield over Young modulus times thickness
- Drawing fails by tearing once blank diameter over punch diameter passes the LDR
Frequently Asked Questions
How do you convert press force into tonnage?
Divide kilonewtons by 9.81 to get kilogram-force, then divide by 1,000, so a 220 kN cut needs about 22 tons, and a safety factor of 15 percent is added for stock variation.
Why does stainless spring back more than mild steel?
Higher yield strength stores more elastic energy before plastic flow begins, and the released curvature grows in direct proportion to that yield strength.
What causes earing on a drawn cup?
Planar anisotropy from rolling makes the rim flow unevenly in the sheet plane, producing scallops that a final trimming pass removes. The ear height is set by the normal anisotropy ratio of the sheet.
Interview Questions
Q1: How do you set punch clearance for a new blanking die?
I start from stock type, use about 8 percent of thickness per side for steel, then check the slug for a clean burnish band and fracture zone.
Q2: How do you control springback in production?
Bottom the punch over a relieved form, or overbend by the computed angle and confirm the first part on a CMM.