Forging, Rolling, and Extrusion Processes
What You'll Learn
- 1Compare open-die, closed-die, and upset forging on force and tooling
- 2Compute true strain, percent reduction, and rolling elongation per pass
- 3Check the rolling bite condition from roll diameter and bite angle
- 4Predict extrusion pressure from the extrusion ratio
Casting gives shape but leaves a random grain structure, while forging, rolling, and extrusion deform solid metal until grains follow the load path. A forged connecting rod may show the same tensile strength as a cast one yet survive far more fatigue cycles, because its grain flow curves around the eye instead of ending at a machined surface. They differ only in how force is applied: forging squeezes a discrete billet, rolling passes strip through rolls, and extrusion pushes a billet through a die. This lesson develops the deformation mathematics common to all three.
Theory and Foundations
All three share one assumption: the metal deforms plastically at constant volume, so area times length is conserved, and elastic recovery is negligible against the plastic strain. The natural measure of deformation is true strain, because it is additive over passes:
where and are the initial and final cross-sections and , are the thicknesses when width is unchanged. Percent reduction, the shop-floor measure, is related to it by
so a reduction of 90 percent corresponds to a true strain of . True strain is preferred because pass strains simply add.
Because flow stress rises with strain, a forming operation sees a mean rather than an endpoint value. Integrating the Hollomon relation over the pass gives
which is the number to multiply by contact area when estimating load.
In forging, the die pressure on a rectangular strip reduced from height to with half-width follows slab analysis:
where is the die-workpiece friction coefficient, near 0.20 for hot steel with glass lubricant and 0.10 for cold steel on phosphated stock. The total forging force is then . The friction term is why a wide, thin part needs disproportionately more force than a tall one of the same volume, and why flash is thinned in closed-die work: the thin flash raises and forces the cavity to fill before the press runs out of stroke.
Rolling converts the same physics into a pass schedule. The draft of a pass is , and the roll can bite only what the contact geometry allows:
where is the roll diameter and is the maximum bite angle, about 30 degrees for grooved rolls and 24 degrees for flat rolls. The projected contact length is
with the roll radius, and the roll force is contact area times mean flow stress, for strip of width . Volume constancy gives the elongation of each pass:
when width spreading is neglected, which holds for strip whose width is at least ten times its thickness.
Extrusion pushes a billet through a die and is characterized by the extrusion ratio
Siebel's formula then predicts the average die pressure as
with constants near and for direct extrusion, reflecting the extra friction of a billet sliding along the container. Indirect extrusion removes that term and typically cuts pressure by 20 to 30 percent. Ratios of 10 to 100 are routine; beyond about 150 the die land runs hot and pressure approaches the press limit.
Key Formulas
Rolling and forging force come from the same flow stress, so the pass load is
and the energy per pass is that force times the distance the metal moves, which for rolling is roll torque times roll angle. Hot working adds a thermal qualifier: recrystallization keeps at zero above roughly 0.6 of the absolute melting temperature, so hot passes show little hardening while cold passes accumulate it fully.
Worked Examples
| Route | Typical tolerance | Strain per pass | Dominant limit |
|---|---|---|---|
| Open-die forging | plus or minus 2 mm | 0.3 to 0.8 | Low volume, labor |
| Closed-die forging | plus or minus 0.4 mm | 0.5 to 1.5 | Die cost, flash loss |
| Hot rolling | plus or minus 0.5 mm | 0.4 to 1.0 | Scale, coarse grain |
| Cold rolling | plus or minus 0.01 mm | 0.1 to 0.3 | Hardening, mill load |
| Hot extrusion | plus or minus 0.2 mm | ln of 10 to 100 | Die life, press force |
Real-World Examples
- Connecting rod - A steel rod is closed-die forged at 1,150 degrees Celsius, flash trimmed, then fracture-split at the cap so the halves reassemble with zero positional error.
- Rail production - A 100 m rail is hot rolled from a 250 mm square bloom in nine passes to a 172 mm height, each pass inside the bite limit.
- Aluminum window section - A 6063-T5 section is extruded at a ratio near 45, then aged at 175 degrees Celsius for 8 hours to reach 150 MPa yield.
- Cold-headed bolt - An M10 head is upset forged cold from wire, roughly doubling tensile strength by work hardening at a true strain near 0.7.
đĄFollow the Grain
Common Mistakes
Assuming hot working adds as much strength as cold
Fix: Hot work only refines grain, strength comes from cold reduction or heat treatment.
Specifying a forged shape with zero draft
Fix: Add 5 to 10 degrees of draft and machine the faces that must sit flat.
Extruding a part whose section varies widely
Fix: Split it into constant profiles, since extrusion cannot step the section along the length.
Key Takeaways
- True strain is the log of the area ratio, and strains from successive passes add
- Mean flow stress K epsilon to the n over n plus one sets forging and rolling load
- Rolling bite fails once draft exceeds D times one minus cos of the bite angle
- Extrusion pressure follows Siebel, so pressure rises with the log of extrusion ratio
Frequently Asked Questions
What is the difference between flash and a flash gutter?
Flash is the thin excess metal squeezed out at the parting line, while the gutter is a deliberate recess that receives it without raising cavity pressure. That thin flash raises friction and forces the cavity to fill.
Why does cold forging raise tensile strength?
Plastic deformation multiplies dislocation density, and those tangled dislocations resist slip, so strength follows upward while elongation falls until annealed.
When should you choose extrusion over rolling?
When the cross-section is constant along the full length. Rolling is economical mainly for shapes a pass schedule can produce, while extrusion makes any constant profile in one operation.
Interview Questions
Q1: How do you decide between hot and cold forging?
I check strength and tolerance together: cold forging gives higher strength and closer size but needs roughly twice the press force.
Q2: What does extrusion ratio tell you?
It sets both property gain and die pressure through ln R, so a ratio far above 150 signals tooling and press risk.